Last updated:

How to print ABS and ASA: a beginner's guide

ABS and ASA are the next step up from PLA and PETG: they handle heat much better, and ASA shrugs off sunlight for outdoor parts. But they warp, they give off fumes, and most open-frame printers aren't a good fit for them. This guide covers what you need before your first spool, how to set up the print, and how to fix the usual problems.

If you're still choosing your first materials, start with PLA vs PETG. PETG already covers most tough or warm-environment parts, and it prints on any printer. Come back here when you need more heat resistance or long-term outdoor use.

ABS vs ASA vs PETG at a glance

Reference numbers from Prusa and Bambu Lab. Always check the range printed on your spool, since brands differ. Heat resistance is Bambu Lab's heat deflection temperature (HDT) for its own filaments, the point where a part starts to sag under light load.

PETG (for comparison)ABSASA
Best forTough everyday partsHeat-resistant technical parts; acetone smoothingOutdoor parts in sun and weather
Heat resistance (Bambu HDT)Higher than PLA's 57 °C87 °C100 °C
UV / outdoor useOKYellows and turns brittle outdoors (Prusa)Very good
Nozzle temperatureAbout 230 to 250 °CPrusa: 255 °C. Bambu: 240 to 280 °CPrusa: 260 °C. Bambu: 240 to 280 °C
Bed temperatureAbout 60 to 90 °CPrusa: about 100 °C (80 to 110). Bambu: 90 to 100 °CPrusa: 105 °C first layer, then 110 °C. Bambu: 90 to 100 °C
EnclosureNot neededNeededNeeded, especially for large parts
FumesNot a styrene materialStrong smell, styreneLess smell than ABS, still styrene
WarpingLowHighHigh, a bit less than ABS

Before you buy a spool: do you have the right setup?

An enclosed printer

ABS and ASA shrink a lot as they cool. If the air around the print is cold or moving, the bottom corners pull up and the layers can split. An enclosure keeps the air warm and still.

Prusa also warns that printing a lot of ABS or ASA in an enclosure can slowly deform plastic printer parts such as the fan shroud. That's mainly a concern for printers that use 3D printed plastic parts.

Ventilation, and where the printer lives

This is the part beginners skip. Both Prusa and Bambu Lab say ABS and ASA release styrene and other potentially harmful substances while printing. Bambu Lab says they can cause dizziness or nausea and gives clear advice:

Prusa adds a catch: ventilate the room, but don't let a draft blow across the printer, because moving air is exactly what makes ABS warp.

If the only place you can print is your bedroom or living room, stick with PLA and PETG. PETG handles more heat than PLA and needs none of this.

Step 1: Dry the spool

Bambu Lab calls ABS and ASA highly hygroscopic (they pull moisture from the air) and recommends drying them before printing. Damp filament gives weaker parts, bubbly surfaces and stringing. Prusa describes ASA as partially hygroscopic.

Step 2: Prepare the build plate (glue is not optional here)

Step 3: Use a real ABS or ASA profile

Pick your brand's ABS or ASA profile in your slicer (Bambu Studio, PrusaSlicer, OrcaSlicer or Cura), or the generic one. Those profiles already use a hot bed, a hot nozzle and little part-cooling fan, because fast cooling makes these materials warp and crack. Change one setting at a time from there. New to slicer settings? See slicer settings explained.

One fix a week, in plain English

Join The First Layer, our free beginner email. Each issue solves one common problem like this one. New subscribers get the free First Print Checklist.

No spam, unsubscribe any time. See our privacy policy.

Step 4: Settings that fight warping

Step 5: Warm the chamber, then print with the door closed

Step 6: Cool down slowly, then remove

Bambu Lab's table says to keep the top glass cover on for ABS and ASA. Opening the door the moment the print finishes cools the part fast, which can make corners lift or layers crack at the last minute. Let it cool inside the closed printer, then remove it once the plate is cool and flex the plate. Still stuck? See how to get a print stuck to the bed off.

Common ABS and ASA problems and quick fixes

What you seeLikely causeTry this
Corners curl up off the platePart cooling and shrinking too fastGlue stick, brim, door and lid closed, preheat the chamber. More in fix warping
Cracks between layers, usually higher upCooling stress is stronger than the layer bondLower the part fan, raise the bed temperature, keep the chamber closed (Bambu Lab). More in how to fix layer separation
Weak, rough or bubbly wallsDamp filament, or nozzle too cold for the speedDry the spool, then raise the nozzle temperature or slow down
Thin, gappy wallsUnder-extrusion or a partial clogSee fix under-extrusion and fix a clogged nozzle
Bottom edge bulges outHot bed plus a squished first layerSee fix elephant's foot
Part doesn't fit, slightly too smallNormal ABS shrinkage (about 1 to 2%)Print a test piece and scale the model slightly
Strong smell in the roomNot enough ventilation or filtrationMove the printer, add ventilation, replace the carbon filter, or switch to PETG

Want stronger parts? Mind the layer direction

ABS and ASA are tougher than PLA side to side, but Bambu Lab's own test data shows their layer bonding (impact strength in the Z direction) is lower than PLA's: 7.4 kJ/m² for ABS and 4.9 kJ/m² for ASA, versus 13.8 kJ/m² for PLA Basic. So orient parts so the force on them doesn't try to peel the layers apart. Bambu Lab recommends thinking about the main direction of force before printing and laying the part out to suit it.

Smoothing ABS and ASA with acetone

One reason people choose ABS and ASA is that acetone vapor can melt the surface into a glossy, nearly layer-free finish. Prusa notes that it also softens sharp edges and fine details, can leave white marks on dark colors, and slightly changes the part's size. Acetone is highly flammable and its vapor can irritate your eyes and lungs, so this is a project for later, done in a well-ventilated area with no flames or sparks nearby and following Prusa's chemical smoothing guide. PLA doesn't smooth with acetone.

Sources

Checked November 10, 2026: Prusa Knowledge Base, ABS and ASA; Prusa blog, Improve your 3D prints with chemical smoothing; Bambu Lab Wiki, ABS / ASA / PC Usage Guide, Filament guide material table, Bambu Studio chamber temperature setting and A1 FAQ.

Your next step

Check the two must-haves first: an enclosed printer and a well-ventilated spot away from where people sleep and relax. If you have both, choose ASA for anything that lives outside, dry the spool, glue the plate, add a brim and print something small and flat to start. If you don't have both, PETG is the better next filament.

Frequently asked questions

Can I print ABS or ASA without an enclosure?

Small parts sometimes work, but it is not recommended. Bambu Lab lists ABS and ASA as requiring an enclosed printer and says its open-frame A1 should only be used for small, low-infill ABS/ASA parts in a well-ventilated space away from people. Prusa says ABS requires an enclosure and ASA needs one for large parts; without one, its draft shield option helps a little.

Is ABS or ASA better for beginners?

ASA is usually the easier of the two. Prusa describes ASA as the successor to ABS: it warps less, smells less and resists UV light, so it holds up outdoors. ABS is often cheaper and smooths well with acetone. Both need the same setup: enclosure, ventilation, glue and a hot bed.

Are ABS and ASA fumes dangerous?

Treat them as a real health concern. Prusa and Bambu Lab both say ABS and ASA release styrene and other potentially harmful substances while printing. Bambu Lab says to avoid printing them in living areas such as bedrooms or living rooms, use ventilation or filtration, and increase ventilation or pause printing if children, pregnant people or anyone with asthma or breathing problems is around.

What temperature should I print ABS and ASA at?

Use the range on your spool. As a reference, Prusa recommends 255 °C nozzle and about 100 °C bed for ABS, and 260 °C nozzle with a 105 °C first layer and 110 °C bed after that for ASA. Bambu Lab lists 240 to 280 °C for the nozzle and 90 to 100 °C for the bed on its plates.

Why do my ABS prints crack between layers?

The part is cooling and shrinking faster than the layers can hold together. Bambu Lab suggests lowering the part cooling fan, raising the bed temperature, and keeping the front door and top lid closed so the chamber stays warm. Under-extrusion from a cold nozzle or a partial clog can cause it too.

Can I print ABS or ASA on a Bambu Lab A1 or with the AMS lite?

Bambu Lab does not recommend it. Its compatibility table says ABS, ASA and PC need an enclosed printer, are not compatible with the P1P or A series, and are not compatible with the AMS lite.

Are ABS and ASA food safe?

Do not assume so. Bambu Lab states that its ABS, ASA and PC filaments are not food-contact grade, and printed layer lines can trap bacteria regardless of material.

One short, friendly email a week: one fix or lesson, one honest pick, and one fun thing to print. New subscribers get the free First Print Checklist.

No spam, unsubscribe any time. See our privacy policy.